dmdesant - posted 12:07, Thursday 28 August 2025 - last comment - 16:52, Friday 29 August 2025(12045)
LASTI SPPKTP Crystal Green Loss/Coating Measurement

Eric, Daniel

We have been constructing a setup to measure the 532nm single-pass transmission and relection coefficients of our new SPPKTP crystals outside of the OPO cavity to confirm the loss estimate from Eric's finesse measurements of the cavities at 532nm. The setup uses a chopper wheel and a lock-in amplifier to remove background light from our measurement. A 150mm focal-length lens is used ahead of the crystal to focus the beam down to a ~100um beam diamater at the center of the crystal.

In this test, we compare the total transmission loss of the least-damaged crystal from the batch (#4) to that of the old LASTI PPKTP crystal which we removed from the cavity a couple weeks ago. In each measurement, the incident beam on the crsytal was aligned as best as possible to the center of the crystal.

New SPPKTP Crystal (#4)

Transmission Measurement (PDA100A Gain = 0dB)

Measurement Voltage (mV) Power (mW)
Lock-In Readout (No XTAL) 323 0.718
Lock-In Readout (w/ XTAL) 314 0.698
  Corresponding Loss 2.79%

Reflection Measurement (PDA36A Gain = 40dB)

Reflection coefficient is calculated relative to estimated incident power from 8% tap PD at the time of the measurement (781uW)

Measurement Voltage (mV) Power Reflected (uW) Reflection Coefficient (ppm)
Lock-In Readout (surface 2 thru 1) 21.3 0.94 1200
Lock-In Readout (surface 1) 21.8 0.96 1230

OLD LASTI PPKTP Crystal

Transmission Measurement (PDA100A Gain = 0dB)

Measurement Voltage (mV) Power (mW)
Lock-In Readout (No XTAL) 313 0.696
Lock-In Readout (w/ XTAL) 307 0.682
  Corresponding Loss 1.92%

Reflection Measurement (PDA36A Gain = 40dB)

Reflection coefficient is calculated relative to estimated incident power from 8% tap PD at the time of the measurement (2.7mW)

Measurement Voltage (mV) Power Reflected (uW) Reflection Coefficient (ppm)
Lock-In Readout (surface 2 thru 1) 1.96 0.087 32?
Lock-In Readout (surface 1) 0.83 0.037 13?

One thing I think we can be certain about is that the old LASTI crsytal has lower overal loss than this new SPPKTP crsytal we measured, which is rather disappointing. The old LASTI crystal's AR coatings are shockingly better than the new SPPKTP's. The reflected beams from the old crystal are super difficult to measure amongst the scatter from the rest of the measurement setup, even with an iris on the reflection detector. As a result, I am not super confident in the accuracy of our reflection coefficients for the old crystal. However, even accouting for the ~0.3% loss from the AR coatings on the new crystal, the SPPKTP crystal specs from Raicon (linked here) would suggest that the total overal loss would be something like (2*0.12%)+1cm*(0.42%/cm) = 0.66%. Our measured loss seems to be more than 4x this amount. On the other hand, the old LASTI crystal's loss (which is seeimngly entirely dominated by bulk losses) is in fact near the specification for the standard Raicon PPKTP crystals (2.2%). Today, I will go back and remeasure this a few times and leave a comment if I can spot a problem with this data.

Images attached to this report
Non-image files attached to this report
Comments related to this report
dmdesant - 18:20, Thursday 28 August 2025 (12047)

I re-measured these again today and found a spot on the new crystal that looks a bit better in terms of transmission losses. I also remeasured the old LASTI crystal for good measure. I also think I had a unit correction missing in the reflection power calculation for the new crystal. Those numbers are in nanowatts (updated to correct), and the same facet was accidentally measured twice (now it seems clear that one facet is almost 2x lower loss than the other). That being said, the reflection coefficients seem to still be correct. In this particular measurement, the old LASTI crystal and the new SPPKTP crsytal are more comparable (around 2% loss).

New SPPKTP Crystal (#4)

Transmission Measurement (PDA100A Gain = 0dB)

Measurement Voltage (mV) Power (mW)
Lock-In Readout (No XTAL) 499 1.11
Lock-In Readout (w/ XTAL) 489 1.09
  Corresponding Loss 2.00%

Reflection Measurement (PDA36A Gain = 40dB)

Reflection coefficient is calculated relative to estimated incident power from 8% tap PD at the time of the measurement (5.06mW)

Measurement Voltage (mV) Power Reflected (uW) Reflection Coefficient (ppm)
Lock-In Readout (left spot) 152 6.71 1330
Lock-In Readout (right spot) 236 10.4 2010

OLD LASTI PPKTP Crystal

Transmission Measurement (PDA100A Gain = 0dB)

Measurement Voltage (mV) Power (mW)
Lock-In Readout (No XTAL) 501 1.09
Lock-In Readout (w/ XTAL) 490 1.11
  Corresponding Loss 2.20%

Reflection Measurement (PDA36A Gain = 40dB)

Reflection coefficient is calculated relative to estimated incident power from 8% tap PD at the time of the measurement (5.10 mW when left spot was measured, 5.16mW when right spot measured)

Measurement Voltage (mV) Power Reflected (uW) Reflection Coefficient (ppm)
Lock-In Readout (left spot) 2.2 0.00971 19?
Lock-In Readout (right spot) 5.4 0.0238 46?
dmdesant - 16:52, Friday 29 August 2025 (12048)

Today, I measured the final crystal that was sitting in the LASTI VOPO. This is XTAL #3 from the SPPKTP batch

New SPPKTP Crystal (#3)

Transmission Measurement (PDA100A Gain = 0dB)

Measurement Voltage (mV) Power (mW)
Lock-In Readout (No XTAL) 505 1.12
Lock-In Readout (w/ XTAL) 499 1.11
  Corresponding Loss 1.19%

Reflection Measurement (PDA36A Gain = 40dB)

Reflection coefficient is calculated relative to estimated incident power from 8% tap PD at the time of the measurement (5.33mW)

Measurement Voltage (mV) Power Reflected (uW) Reflection Coefficient (ppm)
Lock-In Readout (left spot) 245 10.8 2030
Lock-In Readout (right spot) 296 13.1 2450

This crystal actually has about half the loss of XTAL #4, but unfortunately the worst AR coatings yet. That being said, the Raicol-specified loss with these AR coatings should be 0.42% + 0.45% = 0.87%. It seems that the combination of the damage this crystal endured during the coating process and the poor quality coating that resulted likely account for almost half the loss in this sample. We may revisit this crystal in the LASTI VOPO again to see if our initial alignment was at fault for the poor performance we initially saw last week.