Displaying report 1-1 of 1.
Reports until 14:40, Tuesday 19 August 2025
SQZ General
eoelker - posted 14:40, Tuesday 19 August 2025 (12043)
SPPKTP crystal is a dud

[Daniel, Haocun, Eric]

On friday, we decided to swap out the old crystal in the LASTI VOPO with one of the new SPPKTP crystals.  Based on Wen's investigations, we decided to start with crystal #4 from the recent Raicol order, as crystal #3 appears to be damaged along a portion of the ar coated surface.  Before installing the crystal, we decided to change some of the wiring for the oven to address the issues with wire tension causing the solder joints to break.  Seems to be much better now.

Unfortunately the crystal swap doesn't seem to have gone as hoped.  The SPPKTP crystals are supposed to have significantly lower green absorption (<0.5% as opposed to 2.2% with regular PPKTP).  However, the green finnesse doesn't appear to have improved.  I was expecting a value around 250 with the new crystal, but we're still sitting around 140.  Also, the NLG of this crystal seems to be quite low.  Based on our initial measurements, we seem to have a NLG of around 4 with about 11 mW incident and 65% mode coupling.  This corresponds to a threshold power of around 30 mW in TEM00.  Comparing with measured values from O3 (the LASTI VOPO uses the O3 edition of the input/output couplers),  this is much worse than we'd typically see for a new crystal.  Usually a threshold power at this level isn't observed until the crystal is quite old.  A threshold in the 15-20 mW range is more typical for a new spot on a normal PPKTP crystal.  We tried sweeping the temp from about 22C to 40C just to make sure we weren't sitting on a local maximum, but we didn't see much NLG outside of the peak centered at 32.6 C. 

We believe that we are well centered on the crystal and it is well aligned.  We are able to measure a 98% escape efficiency, are seeing 11 coresonance positions across the face of the crystal, and the 532 nm beam appears to be centered on the crystal face.  This is usually a good indication that things are set up properly.

This is quite disappointing.  The lower 532 nm absorption is the reason why Raicol expects them to be more damage resistant.  Given the high losses, I'm not sure if it's worth doing any long-term testing of this crystal.  We will try the 2nd crystal next.  Only a portion of the AR surfaces are damaged, so we should be able to test the remaining regions.  Perhaps we will try to measure the 532 nm AR coating for crystal #4 just to make sure that everything is up to spec.

Displaying report 1-1 of 1.